Issue #7/2025
Y. Aldaiee, D. A. Kuznetsova, M. E. Pirogov, M. V. Kuznetsov, A. A. Popovich
Evaluation of the Effect of Focal Plane Position on the Penetration Depth in Laser Welding of High-strength Steel
Evaluation of the Effect of Focal Plane Position on the Penetration Depth in Laser Welding of High-strength Steel
DOI: 10.22184/1993-7296.FRos.2025.19.7.524.543
The article presents the results of laser welding of steel using the lenses with a focal length of 300, 500, 700 and 900 mm. The effect of focal plane position of laser radiation relative to the work surface of the welded plate on the weld penetration depth has been evaluated. The research is based on a series of experimental welding samples using the lenses with various focal lengths and controlled changes in the focal point relative to the welded plate surface. The results can be used to select the process modes for laser welding of thick high-strength steels and to develop recommendations for the equipment adjustment.
The article presents the results of laser welding of steel using the lenses with a focal length of 300, 500, 700 and 900 mm. The effect of focal plane position of laser radiation relative to the work surface of the welded plate on the weld penetration depth has been evaluated. The research is based on a series of experimental welding samples using the lenses with various focal lengths and controlled changes in the focal point relative to the welded plate surface. The results can be used to select the process modes for laser welding of thick high-strength steels and to develop recommendations for the equipment adjustment.
Теги: focal plane position focusing lenses laser welding penetration depth steel welded joint глубина проплавления лазерная сварка расположение фокальной плоскости сварное соединение сталь фокусирующие линзы
Evaluation of the Effect of Focal Plane Position on the Penetration Depth in Laser Welding of High-strength Steel
Y. Aldaiee, D. A. Kuznetsova, M. E. Pirogov, M. V. Kuznetsov, A. A. Popovich
Peter the Great St. Petersburg Polytechnic University, St. Petersburg, Russia
The article presents the results of laser welding of steel using the lenses with a focal length of 300, 500, 700 and 900 mm. The effect of focal plane position of laser radiation relative to the work surface of the welded plate on the weld penetration depth has been evaluated. The research is based on a series of experimental welding samples using the lenses with various focal lengths and controlled changes in the focal point relative to the welded plate surface. The results can be used to select the process modes for laser welding of thick high-strength steels and to develop recommendations for the equipment adjustment.
Keywords: laser welding, penetration depth, focal plane position, focusing lenses, steel, welded joint
Article received: 28.08.2025
Article accepted: 06.10.2025
INTRODUCTION
Over the past decades, the laser welding (LW) has proved itself as one of the most up-to-date and versatile technologies for joining metallic materials in the modern industry [1–3]. This technology has been highly valued due to its ability to provide the welds with high formation quality, minimal deformation, deep penetration, and a narrow heat-affected zone, as well as the ability to process comprehensive geometric shapes [1, 4–7]. The LW process is specified by the high adaptability and is widely used in various industrial sectors, such as motor vehicle industry, aerospace, electronics, shipbuilding, and energy, where there is a growing demand for the lightweight structures, increased performance, and reliability. The penetrated weld geometry significantly determines the mechanical properties and operating characteristics of the welded joint [8]. The key weld parameters, namely the penetration depth, surface penetration width, cross-sectional shape, and depth-to-width ratio, directly determine the strength, ductility, fatigue life capability, and corrosion resistance of the welded joint [9, 10]. The focal plane position relative to the surface of the material being welded shall be one of the key factors determining the welded joint quality. The correct focal position selection allows for optimization of the penetration depth, weld shape, and reduction of the possible defects such as porosity and cracks [11–14]. The researches demonstrate that the focal plane displacement relative to the material surface significantly affects the energy density distribution of laser radiation (LR) that, in turn, determines the penetration depth and width, as well as the fusion zone configuration [11–15]. When focusing the beam below the surface level, it is possible to achieve the increased penetration depth; however, excessive focus displacement can cause the weld defects and weakening of the joint strength [11, 12, 14]. In addition, the application of lenses with various focal lengths allows for changing the spot diameter and energy distribution that also affects welding geometry and process stability [14, 15].
The modern researches place particular emphasis on a comprehensive analysis of the influence of focal plane position in combination with other process parameters, such as the laser power, welding speed, type of shielding gas, and fiber diameter. This allows for the development of empirical and numerical models for predicting the weld joint geometry and optimizing welding conditions for various steel grades [13–17]. An analysis of the extensive references suggests that the focal plane position significantly determines the weld joint geometry, as it influences the distribution of LR power density on the surface of the welded samples [18–22].
The resulting weld quality is significantly affected by a number of factors: welding heat input, composition and consumption of the shielding gas, as well as the beam focusing conditions and power density. Among these parameters, the focal plane displacement relative to the welded surface is of particular importance. Even small changes in this parameter can significantly alter the energy distribution in the beam impact area that, in turn, affects the molten pool stability and, consequently, the achievable penetration depth [21]. The experimental studies confirm that in order to achieve optimal penetration depth, it is necessary to maintain a certain position of the focal plane relative to the workpiece surface [23–26]. The theoretical models and numerical simulations further elucidate such relations while indicating that the final result is also affected by the LR power, welding speed, beam diameter, and the thermophysical properties of steel [27].
The modern laser welding systems apply various types of focusing lenses with different focal lengths. Each focal length provides for a specific intensity distribution in the focal area that is characterized by the focal spot diameter, beam convergence angle, and a depth of field. Such optical parameters significantly affect the processes of energy absorption, metal melting, and keyhole generation in the welding zone [28]. The lenses with a short focal length provide a small focal spot diameter and high power density, but have a shallow depth of field and are highly sensitive to the positioning accuracy [29]. The lenses with a greater focal length produce a larger focal spot but a greater depth of field while being less sensitive to the focus offsets [30]. Accurate positioning of the focal plane ensures the most efficient use of LR energy, reduces the energy consumption level, and accelerates the welding process. This is especially important when welding steel structures of varying thicknesses, where the requirements for penetration depth, weld quality, and performance can vary significantly depending on the specific application.
Despite the significant advances in the field of LW of metals, the quantitative influence of the focal plane position on the geometric specifications of the welded seam is still insufficiently systematized. Most existing studies focus on the optimization of parameters, such as the LR power, welding speed, shielding gas composition, and surface preparation of the material [31–34]. Moreover, precise positioning of the focal plane and the use of lenses with various focal lengths require more in-depth theoretical analysis and experimental validation. Therefore, the study of influence of the focal plane position and optical specifications on the penetration weld seam geometry is a pressing issue for improving the quality and reliability of laser welded joints.
The aim of the research is a systematic experimental assessment and theoretical justification of the influence of focal plane position on the welded seam penetration depth in the case of LW of thick high-strength steel using the lenses with different focal lengths.
1. EXPERIMENTAL EQUIPMENT
The works on development of the LW mode, as well as welding of the test samples, have been performed using a robotic process system for hybrid laser-arc welding (RPS HLAW) in the research laboratory “Laser and Additive Technologies”, of the Institute of Mechanical Engineering, Materials and Transport at Peter the Great St. Petersburg Polytechnic University (Fig. 1).
For the safety reasons, the RPS HLAW is placed in a protective cabin, preventing the dangerous effects of reflected LR. The cabin is equipped with the windows, light filters, video surveillance cameras, and ventilation. The RPS HLAW composition is given in Table 1. The laser source parameters are listed in Table 2. The beam caustic is shown in Figure 2.
2. EXPERIMENTATION
2.1. Determination of the Focal Plane Position of Laser Radiation
As a part of the research, the work has been carried out to determine the focal plane position of the LR relative to the laser head in the pulse mode (laser power P = 40 W, pulse time t = 0,05 s) for the lenses with a focal length of 300, 500, 700 and 900 mm. The schematic diagram for determining the focal plane position in the pulse mode is shown in Fig. 3.
The plates with an attached photopaper have been used for testing (Fig. 4). The print diameter for all lenses has been determined using an inverted optical microscope IM7400L (Meiji Techno, Japan) (Fig. 5, a). As a result, the minimum diameters of the prints have been determined for all lenses (Fig. 5, b, c, d and e). Based on Fig. 5 it is clear that the lenses with a shorter focal length provide a smaller and more concentrated spot, while those with a longer focal length provide a larger and less intense spot.
During the experiment, to accurately determine the print diameter, the diameters of three prints D1, D2, D3 made at the same focal length have been measured for each lens (see Fig. 4) according to the formula Dn = (Dn, h + Dn, v) / 2 where Dn, h is the horizontal measurement of the print, Dn, v is the vertical measurement of the print. and then the arithmetic mean of the measurement values has been calculated Dav = (D1 + D2 + D3) / 3. After analyzing the results, the dependence of the print diameter D1, D2, D3 and Dav on the focal plane offset dF from the processed surface of the plate for all lenses has been constructed (Fig. 6). It can be noted that the distance from the laser head cutoff to the surface of the plate H with the smallest print diameter (focal plane) is H = 238 mm – for the lens 300 mm, H = 440 mm – for the lens 500 mm, H = 656 mm – for the lens 700 mm, H = 849 mm – for the lens 900 mm.
Figure 6 shows that for all lenses, the print diameter is gradually increased with displacement from the focal plane that is a typical manifestation of defocusing due to the beam energy scattering and enlargement of the spot. All curves are close to the V-curve and almost symmetrical relative to dF = 0.
2.2. Experimental Results Processing Using the Approximation Function Method
The experimental points (xi,yi) ~ (Hi, Di) of three experiments for all lenses can be approximated by the function (Fig. 7). A linear approximating function has been proposed, containing a vector of variable parameters p that are found by the least squares method:
F(p) = ωn Dexp. n − Dcalc.(p, Hn)2 → min, (1)
where F is the objective function, ωn is the weight of experiment.
We have divided the set of experiments for each lens into two parts: before and after the spot with the minimum diameter. As a result, two approximating functions for each lens have been obtained, which describe the points of the experiments. Figure 8 illustrates the experimental points and the corresponding approximation curves (functions of the same type at ωn = 1) for all lenses:
D(a, b, H) = a ∙ H + b, (2)
where the unknown parameters a, b are the solution to the optimization problem with the following objective function:
F(a, b) = Dn − D(a, b, Hn)2 → min. (3)
Figure 8 also shows the 95% prediction range for the experimental points (gray background in Figure 8). This is the range of values within which, a new data point shall fall with 95% probability under the same experimental conditions (due to the variability in observations themselves and measurement errors).
The approximation functions that describe the curves (Fig. 8, red curves) for all lenses are given in Table 3. To verify the experimental results, the intersection point of two curves for each lens can be found (see Fig. 8, red curves). The physical meaning of the intersection point is (Hcalc., Dcalc.), where Hcalc. is the calculated distance from the laser head cutoff to the welded plate surface with the smallest diameter of the print (focal plane); Dcalc. is the calculated smallest diameter of the print.
For the lens 300 mm the calculated distance Hcalc. can be found as follows:
D1 = D2 ⇒ a1 Hcalc. + b1 = a2 Hcalc. + b2 ⇒ Hcalc. =
75.464 Hcalc. − 17 433.011 = −69.381 Hcalc. + 17 005.52
⇒ Hcalc. = = 237,761 mm.
The calculation has been repeated for all lenses, and all the results are presented in Table 3.
It is possible to calculate the relative error EH between the experimental Hexp. and calculated Hcalc. values: for the lens 300 mm relative error EH of the distance from the laser head cutoff to the welded plate surface can be calculated as follows:
| EH | = × 100% =
= × 100% = 0,100%.
The calculation has been repeated for all lenses, and all the results are presented in Table 4. Data analysis shows satisfactory agreement between the calculated Hсalc. and experimental Hexp. values.
3. EFFECT OF THE FOCAL PLANE DISPLACEMENT
ON THE PENETRATION DEPTH
The focal plane displacement during the LW process affects the power distribution in the affected zone. This fact typically changes the penetrated weld geometry. To evaluate the effect of focal plane displacement on the weld penetration depth in the downhand position, the welds have been made on two plates with the dimensions of 500 ×2 50 × 50 mm made of high-strength steel in the down-thrust position (Fig. 9, a and b). The plates have been cut into pieces for grinding, analysis and measurement of the penetration depth of each weld (Fig. 9, c). The dependence of the penetration depth h on the focus displacement dF has been registered.
The welds have been made using the lenses 300, 500, 700 and 900 mm (Fig. 9). The LW mode for all samples has been as follows: laser power P = 20 kW, welding speed v = 20 mm s−1, Ar gas consumption R = 25 L min−1 displacement of the focal plane from the work surface of the welded plate dF = [+4, −18]. The focal plane displacement from the processed surface of the welded plate and the corresponding penetration depths for all lenses are given in Table 5. The weld sections using the lenses 300, 500, 700 and 900 mm are shown in Fig. 10.
3.1. Discussion of results
For the lens 300 mm, the dependence of penetration depth h on the focus displacement dF is characterized by the significant fluctuations: the distinct peaks and troughs are observed. The maximum penetration depth hmax = 32 mm at dF = −12 mm, and the minimum penetration depth hmin = 17 mm is provided at dF = +2 mm (Fig. 11, a). The range of changes in the penetration depth h is rather large, and the local variations in terms of dF are sharp. For the lens 500 mm, the dependence h(dF) has a smoother appearance, while the distinct peaks and troughs are also preserved: the maximum penetration depth hmax = 32 mm is provided at dF = −18 mm, and the minimum penetration depth is hmin = 20 mm given at dF = +4 mm (Fig. 11, b). A general trend towards a decrease in depth is observed with a positive focus displacement. For the lens 700 mm, the dependence h(dF) becomes even smoother compared to 300 and 500 mm: the amplitude of oscillations decreases, while the maximum depth reaches hmax = 24 mm at dF = −10 mm, and the minimum penetration depth hmin = 17 mm is provided at dF = +2 mm (Fig. 11, c). The local variations are moderately expressed. For the lens 900 mm, the dependence h(dF) is most even, and the sensitivity h to the changes dF is minimal. The maximum penetration depth hmax = 22 mm is provided at dF = +2 mm, and the minimum penetration depth hmin = 14 mm is ensured at dF = −14 mm (Fig. 11, d).
During the welding with the lenses 300 and 500 mm, the maximum penetration depths values are achieved with a negative focal displacement. This is due to the fact that focusing below the surface increases the power density within the material, stabilizes the keyhole, and directs the heat flow inward, while ensuring deeper penetration. In the case of a positive focal displacement (focusing above the surface), the spot diameter on the surface is increased, the power density is reduced, and the LR is dissipated closer to the surface that leads to а decrease in penetration depth. In the case of negative displacement, instability of the values (peaks and troughs) is observed that can be associated with the keyhole instability, its periodic collapse, and changes in the melt pool geometry; this phenomenon is accompanied by changes in the conditions of heat and mass transfer in the pool. The application of lenses with the focal lengths of 700 and 900 mm ensures a smoother dependence of penetration depth on the focal plane displacement compared to the lenses with a shorter focal length. The amplitude of oscillations h is approximately 17–24 mm for a lens 700 mm and 14–22 mm for a lens 900 mm that is less than for the lenses 300 and 500 mm. This fact indicates that increasing the focal length reduces the system sensitivity to the penetration depth variations and stabilizes the focal plane position. However, simultaneously, the maximum penetration depth is decreased; in addition, with increasing focal length, the waist length increases.
To achieve greater weld penetration depth, it is advisable to use lenses with a shorter focal length (300 and 500 mm). However, if the process stability and weld uniformity with the possible small focus displacements are a priority, the long-focus lenses (700 and 900 mm) are preferable.
CONCLUSIONS
Based on the results of print measurements, the focal point has been determined, at which the distances from the laser head cutoff to the plate surface were Hexp. = 238 mm for the lens 300 mm, Hexp. = 440 mm for the lens 500 mm, Hexp. = 656 mm for the lens 700 mm, Hexp. = 849 mm for the lens 900 mm. After the experimental data processing and prediction of the approximation function, the calculated values Hcalc..have been obtained. The coincidence between the experimental Hexp. and calculated Hcalc. values is satisfactory.
The maximum penetration depth reaches 32 mm by using a lens 300 mm with a focal plane offset from the work surface of the welded plate dF = −12 mm, 32 mm by using a lens 500 mm with dF = −18 mm, 24 mm by using a lens 700 mm with dF = −10 mm and 22 mm by using a lens 900 mm with dF = +2 mm.
The short focus lenses (300 and 500 mm) provide the higher power density and, therefore, greater maximum penetration depth. However, they place more stringent demands on the accuracy of focal plane positioning.
The long focus lenses (700 and 900 mm) are characterized by a greater depth of field that reduces the process sensitivity to the small focal plane displacements, but their maximum surface power density is lower than that of the short focal length lenses.
The increased focal length reduces the system’s sensitivity to the penetration depth variations and stabilizes the focal plane position, but the maximum penetration depth is simultaneously decreased.
Based on the work results, it is scheduled to develop a hybrid laser-arc welding technology for butt joints with a root face height of at least 32 mm.
ACKNOWLEDGEMENTS
The research has been performed with financial support of the Ministry of Science and Higher Education of the Russian Federation as a part of the strategic academic leadership program “Priority 2030” (Agreement No. 075-15-2025-210 dated 04 April 2025).
AUTHORS
Aldaiee Yarob, engineer of the research laboratory “Laser and Additive Technologies”, Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: hybrid laser-arc welding, laser welding, physical processes in materials during welding, phase and structural transformations, hydrogen diffusion and cold cracking in welding, stresses and deformations in welding and related processes. E-mail: aldaiee.yarob@gmail.com.
ORCID: 0009-0000-7968-668X
Kuznetsova Daria A., engineer of the research laboratory “Laser and Additive Technologies”, Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: study of the structure and properties of casting alloys, technologies for obtaining and modifying nanomaterials and coatings, microstructural analysis. E-mail: kuznetsova_da@spbstu.ru.
ORCID: 0009-0003-3938-5710
Pirogov Maksim E., engineer of the research laboratory “Laser and Additive Technologies”, Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: hybrid laser-arc welding, laser welding, additive technologies. E-mail: maks.pirogov2000@mail.ru.
ORCID: 0009-0006-7374-4635
Kuznetsov Mikhail V., Cand. of Sc. (Techn.), Head of the Research Laboratory “Laser and Additive Technologies”, Director of the Russian-German Center for Laser Technologies, Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: hybrid laser-arc welding, laser welding, additive technologies, laser cladding, direct laser deposition. E-mail: kuznetsov_mich@mail.ru.
ORCID: 0000-0002-9981-1078
Popovich Anatoly A., Dr. of Sc. (Techn.), professor, director of the Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: development of theoretical fundamentals and efficient technologies for obtaining powders of refractory compounds and related alloys in the conditions of high-temperature mechanochemical synthesis, development of new anode and cathode materials for lithium-ion polymer batteries, additive technologies. E-mail: director@immet.spbstu.ru.
ORCID: 0000-0002-5974-6654
CONFLICT OF INTEREST STATEMENT
The authors confirm that they have no known financial or personal conflicts of interest that could have influenced the research presented in this manuscript.
Y. Aldaiee, D. A. Kuznetsova, M. E. Pirogov, M. V. Kuznetsov, A. A. Popovich
Peter the Great St. Petersburg Polytechnic University, St. Petersburg, Russia
The article presents the results of laser welding of steel using the lenses with a focal length of 300, 500, 700 and 900 mm. The effect of focal plane position of laser radiation relative to the work surface of the welded plate on the weld penetration depth has been evaluated. The research is based on a series of experimental welding samples using the lenses with various focal lengths and controlled changes in the focal point relative to the welded plate surface. The results can be used to select the process modes for laser welding of thick high-strength steels and to develop recommendations for the equipment adjustment.
Keywords: laser welding, penetration depth, focal plane position, focusing lenses, steel, welded joint
Article received: 28.08.2025
Article accepted: 06.10.2025
INTRODUCTION
Over the past decades, the laser welding (LW) has proved itself as one of the most up-to-date and versatile technologies for joining metallic materials in the modern industry [1–3]. This technology has been highly valued due to its ability to provide the welds with high formation quality, minimal deformation, deep penetration, and a narrow heat-affected zone, as well as the ability to process comprehensive geometric shapes [1, 4–7]. The LW process is specified by the high adaptability and is widely used in various industrial sectors, such as motor vehicle industry, aerospace, electronics, shipbuilding, and energy, where there is a growing demand for the lightweight structures, increased performance, and reliability. The penetrated weld geometry significantly determines the mechanical properties and operating characteristics of the welded joint [8]. The key weld parameters, namely the penetration depth, surface penetration width, cross-sectional shape, and depth-to-width ratio, directly determine the strength, ductility, fatigue life capability, and corrosion resistance of the welded joint [9, 10]. The focal plane position relative to the surface of the material being welded shall be one of the key factors determining the welded joint quality. The correct focal position selection allows for optimization of the penetration depth, weld shape, and reduction of the possible defects such as porosity and cracks [11–14]. The researches demonstrate that the focal plane displacement relative to the material surface significantly affects the energy density distribution of laser radiation (LR) that, in turn, determines the penetration depth and width, as well as the fusion zone configuration [11–15]. When focusing the beam below the surface level, it is possible to achieve the increased penetration depth; however, excessive focus displacement can cause the weld defects and weakening of the joint strength [11, 12, 14]. In addition, the application of lenses with various focal lengths allows for changing the spot diameter and energy distribution that also affects welding geometry and process stability [14, 15].
The modern researches place particular emphasis on a comprehensive analysis of the influence of focal plane position in combination with other process parameters, such as the laser power, welding speed, type of shielding gas, and fiber diameter. This allows for the development of empirical and numerical models for predicting the weld joint geometry and optimizing welding conditions for various steel grades [13–17]. An analysis of the extensive references suggests that the focal plane position significantly determines the weld joint geometry, as it influences the distribution of LR power density on the surface of the welded samples [18–22].
The resulting weld quality is significantly affected by a number of factors: welding heat input, composition and consumption of the shielding gas, as well as the beam focusing conditions and power density. Among these parameters, the focal plane displacement relative to the welded surface is of particular importance. Even small changes in this parameter can significantly alter the energy distribution in the beam impact area that, in turn, affects the molten pool stability and, consequently, the achievable penetration depth [21]. The experimental studies confirm that in order to achieve optimal penetration depth, it is necessary to maintain a certain position of the focal plane relative to the workpiece surface [23–26]. The theoretical models and numerical simulations further elucidate such relations while indicating that the final result is also affected by the LR power, welding speed, beam diameter, and the thermophysical properties of steel [27].
The modern laser welding systems apply various types of focusing lenses with different focal lengths. Each focal length provides for a specific intensity distribution in the focal area that is characterized by the focal spot diameter, beam convergence angle, and a depth of field. Such optical parameters significantly affect the processes of energy absorption, metal melting, and keyhole generation in the welding zone [28]. The lenses with a short focal length provide a small focal spot diameter and high power density, but have a shallow depth of field and are highly sensitive to the positioning accuracy [29]. The lenses with a greater focal length produce a larger focal spot but a greater depth of field while being less sensitive to the focus offsets [30]. Accurate positioning of the focal plane ensures the most efficient use of LR energy, reduces the energy consumption level, and accelerates the welding process. This is especially important when welding steel structures of varying thicknesses, where the requirements for penetration depth, weld quality, and performance can vary significantly depending on the specific application.
Despite the significant advances in the field of LW of metals, the quantitative influence of the focal plane position on the geometric specifications of the welded seam is still insufficiently systematized. Most existing studies focus on the optimization of parameters, such as the LR power, welding speed, shielding gas composition, and surface preparation of the material [31–34]. Moreover, precise positioning of the focal plane and the use of lenses with various focal lengths require more in-depth theoretical analysis and experimental validation. Therefore, the study of influence of the focal plane position and optical specifications on the penetration weld seam geometry is a pressing issue for improving the quality and reliability of laser welded joints.
The aim of the research is a systematic experimental assessment and theoretical justification of the influence of focal plane position on the welded seam penetration depth in the case of LW of thick high-strength steel using the lenses with different focal lengths.
1. EXPERIMENTAL EQUIPMENT
The works on development of the LW mode, as well as welding of the test samples, have been performed using a robotic process system for hybrid laser-arc welding (RPS HLAW) in the research laboratory “Laser and Additive Technologies”, of the Institute of Mechanical Engineering, Materials and Transport at Peter the Great St. Petersburg Polytechnic University (Fig. 1).
For the safety reasons, the RPS HLAW is placed in a protective cabin, preventing the dangerous effects of reflected LR. The cabin is equipped with the windows, light filters, video surveillance cameras, and ventilation. The RPS HLAW composition is given in Table 1. The laser source parameters are listed in Table 2. The beam caustic is shown in Figure 2.
2. EXPERIMENTATION
2.1. Determination of the Focal Plane Position of Laser Radiation
As a part of the research, the work has been carried out to determine the focal plane position of the LR relative to the laser head in the pulse mode (laser power P = 40 W, pulse time t = 0,05 s) for the lenses with a focal length of 300, 500, 700 and 900 mm. The schematic diagram for determining the focal plane position in the pulse mode is shown in Fig. 3.
The plates with an attached photopaper have been used for testing (Fig. 4). The print diameter for all lenses has been determined using an inverted optical microscope IM7400L (Meiji Techno, Japan) (Fig. 5, a). As a result, the minimum diameters of the prints have been determined for all lenses (Fig. 5, b, c, d and e). Based on Fig. 5 it is clear that the lenses with a shorter focal length provide a smaller and more concentrated spot, while those with a longer focal length provide a larger and less intense spot.
During the experiment, to accurately determine the print diameter, the diameters of three prints D1, D2, D3 made at the same focal length have been measured for each lens (see Fig. 4) according to the formula Dn = (Dn, h + Dn, v) / 2 where Dn, h is the horizontal measurement of the print, Dn, v is the vertical measurement of the print. and then the arithmetic mean of the measurement values has been calculated Dav = (D1 + D2 + D3) / 3. After analyzing the results, the dependence of the print diameter D1, D2, D3 and Dav on the focal plane offset dF from the processed surface of the plate for all lenses has been constructed (Fig. 6). It can be noted that the distance from the laser head cutoff to the surface of the plate H with the smallest print diameter (focal plane) is H = 238 mm – for the lens 300 mm, H = 440 mm – for the lens 500 mm, H = 656 mm – for the lens 700 mm, H = 849 mm – for the lens 900 mm.
Figure 6 shows that for all lenses, the print diameter is gradually increased with displacement from the focal plane that is a typical manifestation of defocusing due to the beam energy scattering and enlargement of the spot. All curves are close to the V-curve and almost symmetrical relative to dF = 0.
2.2. Experimental Results Processing Using the Approximation Function Method
The experimental points (xi,yi) ~ (Hi, Di) of three experiments for all lenses can be approximated by the function (Fig. 7). A linear approximating function has been proposed, containing a vector of variable parameters p that are found by the least squares method:
F(p) = ωn Dexp. n − Dcalc.(p, Hn)2 → min, (1)
where F is the objective function, ωn is the weight of experiment.
We have divided the set of experiments for each lens into two parts: before and after the spot with the minimum diameter. As a result, two approximating functions for each lens have been obtained, which describe the points of the experiments. Figure 8 illustrates the experimental points and the corresponding approximation curves (functions of the same type at ωn = 1) for all lenses:
D(a, b, H) = a ∙ H + b, (2)
where the unknown parameters a, b are the solution to the optimization problem with the following objective function:
F(a, b) = Dn − D(a, b, Hn)2 → min. (3)
Figure 8 also shows the 95% prediction range for the experimental points (gray background in Figure 8). This is the range of values within which, a new data point shall fall with 95% probability under the same experimental conditions (due to the variability in observations themselves and measurement errors).
The approximation functions that describe the curves (Fig. 8, red curves) for all lenses are given in Table 3. To verify the experimental results, the intersection point of two curves for each lens can be found (see Fig. 8, red curves). The physical meaning of the intersection point is (Hcalc., Dcalc.), where Hcalc. is the calculated distance from the laser head cutoff to the welded plate surface with the smallest diameter of the print (focal plane); Dcalc. is the calculated smallest diameter of the print.
For the lens 300 mm the calculated distance Hcalc. can be found as follows:
D1 = D2 ⇒ a1 Hcalc. + b1 = a2 Hcalc. + b2 ⇒ Hcalc. =
75.464 Hcalc. − 17 433.011 = −69.381 Hcalc. + 17 005.52
⇒ Hcalc. = = 237,761 mm.
The calculation has been repeated for all lenses, and all the results are presented in Table 3.
It is possible to calculate the relative error EH between the experimental Hexp. and calculated Hcalc. values: for the lens 300 mm relative error EH of the distance from the laser head cutoff to the welded plate surface can be calculated as follows:
| EH | = × 100% =
= × 100% = 0,100%.
The calculation has been repeated for all lenses, and all the results are presented in Table 4. Data analysis shows satisfactory agreement between the calculated Hсalc. and experimental Hexp. values.
3. EFFECT OF THE FOCAL PLANE DISPLACEMENT
ON THE PENETRATION DEPTH
The focal plane displacement during the LW process affects the power distribution in the affected zone. This fact typically changes the penetrated weld geometry. To evaluate the effect of focal plane displacement on the weld penetration depth in the downhand position, the welds have been made on two plates with the dimensions of 500 ×2 50 × 50 mm made of high-strength steel in the down-thrust position (Fig. 9, a and b). The plates have been cut into pieces for grinding, analysis and measurement of the penetration depth of each weld (Fig. 9, c). The dependence of the penetration depth h on the focus displacement dF has been registered.
The welds have been made using the lenses 300, 500, 700 and 900 mm (Fig. 9). The LW mode for all samples has been as follows: laser power P = 20 kW, welding speed v = 20 mm s−1, Ar gas consumption R = 25 L min−1 displacement of the focal plane from the work surface of the welded plate dF = [+4, −18]. The focal plane displacement from the processed surface of the welded plate and the corresponding penetration depths for all lenses are given in Table 5. The weld sections using the lenses 300, 500, 700 and 900 mm are shown in Fig. 10.
3.1. Discussion of results
For the lens 300 mm, the dependence of penetration depth h on the focus displacement dF is characterized by the significant fluctuations: the distinct peaks and troughs are observed. The maximum penetration depth hmax = 32 mm at dF = −12 mm, and the minimum penetration depth hmin = 17 mm is provided at dF = +2 mm (Fig. 11, a). The range of changes in the penetration depth h is rather large, and the local variations in terms of dF are sharp. For the lens 500 mm, the dependence h(dF) has a smoother appearance, while the distinct peaks and troughs are also preserved: the maximum penetration depth hmax = 32 mm is provided at dF = −18 mm, and the minimum penetration depth is hmin = 20 mm given at dF = +4 mm (Fig. 11, b). A general trend towards a decrease in depth is observed with a positive focus displacement. For the lens 700 mm, the dependence h(dF) becomes even smoother compared to 300 and 500 mm: the amplitude of oscillations decreases, while the maximum depth reaches hmax = 24 mm at dF = −10 mm, and the minimum penetration depth hmin = 17 mm is provided at dF = +2 mm (Fig. 11, c). The local variations are moderately expressed. For the lens 900 mm, the dependence h(dF) is most even, and the sensitivity h to the changes dF is minimal. The maximum penetration depth hmax = 22 mm is provided at dF = +2 mm, and the minimum penetration depth hmin = 14 mm is ensured at dF = −14 mm (Fig. 11, d).
During the welding with the lenses 300 and 500 mm, the maximum penetration depths values are achieved with a negative focal displacement. This is due to the fact that focusing below the surface increases the power density within the material, stabilizes the keyhole, and directs the heat flow inward, while ensuring deeper penetration. In the case of a positive focal displacement (focusing above the surface), the spot diameter on the surface is increased, the power density is reduced, and the LR is dissipated closer to the surface that leads to а decrease in penetration depth. In the case of negative displacement, instability of the values (peaks and troughs) is observed that can be associated with the keyhole instability, its periodic collapse, and changes in the melt pool geometry; this phenomenon is accompanied by changes in the conditions of heat and mass transfer in the pool. The application of lenses with the focal lengths of 700 and 900 mm ensures a smoother dependence of penetration depth on the focal plane displacement compared to the lenses with a shorter focal length. The amplitude of oscillations h is approximately 17–24 mm for a lens 700 mm and 14–22 mm for a lens 900 mm that is less than for the lenses 300 and 500 mm. This fact indicates that increasing the focal length reduces the system sensitivity to the penetration depth variations and stabilizes the focal plane position. However, simultaneously, the maximum penetration depth is decreased; in addition, with increasing focal length, the waist length increases.
To achieve greater weld penetration depth, it is advisable to use lenses with a shorter focal length (300 and 500 mm). However, if the process stability and weld uniformity with the possible small focus displacements are a priority, the long-focus lenses (700 and 900 mm) are preferable.
CONCLUSIONS
Based on the results of print measurements, the focal point has been determined, at which the distances from the laser head cutoff to the plate surface were Hexp. = 238 mm for the lens 300 mm, Hexp. = 440 mm for the lens 500 mm, Hexp. = 656 mm for the lens 700 mm, Hexp. = 849 mm for the lens 900 mm. After the experimental data processing and prediction of the approximation function, the calculated values Hcalc..have been obtained. The coincidence between the experimental Hexp. and calculated Hcalc. values is satisfactory.
The maximum penetration depth reaches 32 mm by using a lens 300 mm with a focal plane offset from the work surface of the welded plate dF = −12 mm, 32 mm by using a lens 500 mm with dF = −18 mm, 24 mm by using a lens 700 mm with dF = −10 mm and 22 mm by using a lens 900 mm with dF = +2 mm.
The short focus lenses (300 and 500 mm) provide the higher power density and, therefore, greater maximum penetration depth. However, they place more stringent demands on the accuracy of focal plane positioning.
The long focus lenses (700 and 900 mm) are characterized by a greater depth of field that reduces the process sensitivity to the small focal plane displacements, but their maximum surface power density is lower than that of the short focal length lenses.
The increased focal length reduces the system’s sensitivity to the penetration depth variations and stabilizes the focal plane position, but the maximum penetration depth is simultaneously decreased.
Based on the work results, it is scheduled to develop a hybrid laser-arc welding technology for butt joints with a root face height of at least 32 mm.
ACKNOWLEDGEMENTS
The research has been performed with financial support of the Ministry of Science and Higher Education of the Russian Federation as a part of the strategic academic leadership program “Priority 2030” (Agreement No. 075-15-2025-210 dated 04 April 2025).
AUTHORS
Aldaiee Yarob, engineer of the research laboratory “Laser and Additive Technologies”, Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: hybrid laser-arc welding, laser welding, physical processes in materials during welding, phase and structural transformations, hydrogen diffusion and cold cracking in welding, stresses and deformations in welding and related processes. E-mail: aldaiee.yarob@gmail.com.
ORCID: 0009-0000-7968-668X
Kuznetsova Daria A., engineer of the research laboratory “Laser and Additive Technologies”, Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: study of the structure and properties of casting alloys, technologies for obtaining and modifying nanomaterials and coatings, microstructural analysis. E-mail: kuznetsova_da@spbstu.ru.
ORCID: 0009-0003-3938-5710
Pirogov Maksim E., engineer of the research laboratory “Laser and Additive Technologies”, Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: hybrid laser-arc welding, laser welding, additive technologies. E-mail: maks.pirogov2000@mail.ru.
ORCID: 0009-0006-7374-4635
Kuznetsov Mikhail V., Cand. of Sc. (Techn.), Head of the Research Laboratory “Laser and Additive Technologies”, Director of the Russian-German Center for Laser Technologies, Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: hybrid laser-arc welding, laser welding, additive technologies, laser cladding, direct laser deposition. E-mail: kuznetsov_mich@mail.ru.
ORCID: 0000-0002-9981-1078
Popovich Anatoly A., Dr. of Sc. (Techn.), professor, director of the Institute of Mechanical Engineering, Materials and Transport, Federal Autonomous Educational Institution of Higher Education “Peter the Great St. Petersburg Polytechnic University”, Saint-Petersburg, Russia. Research interests: development of theoretical fundamentals and efficient technologies for obtaining powders of refractory compounds and related alloys in the conditions of high-temperature mechanochemical synthesis, development of new anode and cathode materials for lithium-ion polymer batteries, additive technologies. E-mail: director@immet.spbstu.ru.
ORCID: 0000-0002-5974-6654
CONFLICT OF INTEREST STATEMENT
The authors confirm that they have no known financial or personal conflicts of interest that could have influenced the research presented in this manuscript.
Readers feedback
rus